Nanostructured Electrolytic Composites Based on Cobalt Alloys …
739
Table 1 (continued)
Specimen # Mode
Composition (in the
terms of metal)
SEM magnification ×5000
6
4 A/dm 2 ;
t on /t off = 2 ms/10 ms
wt%:
Co—88.25;
W—9.06;
Zr—2.69
7
6 A/dm 2 ;
t on /t off = 2 ms/10 ms
wt%:
Co—73.87;
W—24.35;
Zr—1.78
8
3 A/dm 2
at.%:
Fe—51;
Co—36;
Mo—13
9
3 A/dm 2 ;
t on /t off = 2 ms/5 ms
at.%:
Fe—50;
Co—39;
Mo—11
10
5 A/dm 2 ;
t on /t off = 2 ms/5 ms
at.%:
Fe—51;
Co—40;
Mo—9