738
M. Ved’ et al.
Table 1 Deposition modes, composition, and morphology of the surface of ternary cobalt alloys
Specimen # Mode
Composition (in the
terms of metal)
SEM magnification ×5000
1
4 A/dm 2 ;
t on /t off = 2 ms/10 ms
wt%:
Co—59.94;
Mo—23.28;
W—16.77
2
6 A/dm 2 ;
t on /t off = 2 ms/10 ms
wt%:
Co—61.06;
Mo—20.58;
W—18.36
3
4 A/dm 2 ;
t on /t off = 2 ms/10 ms
wt%:
Co—62.13;
M—33.29;
Zr—4.58
4
4 A/dm 2 ;
t on /t off = 5 ms/10 ms
wt%:
Co—63.61;
Mo—32.60;
Zr—3.79
5
6 A/dm 2 ;
t on /t off = 5 ms/10 ms
wt%:
Co—68.96;
Mo—26.68;
Zr—4.36
(continued)